PCC starts as limestone and ends as limestone: about 77% calcium carbonate on average (dry basis), finely precipitated, and ready to displace virgin quarried material. It is a circular, cost-effective carbonate that replaces virgin limestone in Type IL cement (raw and finish mill applications), ready-mix concrete, and concrete leveling and repair, sourced from four Rocky Mountain and High Plains factories.
Chemical and physical profile
PCC is calcium carbonate, the same compound cement plants already use in two places: as raw-meal feed to the kiln, and as the limestone interground at the finish mill to make Type IL portland-limestone cement. Unlike quarry rock, PCC arrives pre-processed, with no crushing required. It is already as fine as the limestone fraction a cement plant spends on grinding power to produce, or that a ready-mix producer or concrete leveling company buys as a mineral filler, and it has about twice the ultrafine (<2 µm) content of portland cement. PCC values come from independent laboratory testing of multiple samples.
Calcium carbonate (CaCO₃)
CaO equivalent (calculated)
Loss on ignition (LOI) at 950 °C
*Pure calcium carbonate can lose no more than 44.0% on ignition, all of it as CO₂. PCC’s higher LOI includes roughly 10–17% of the dry weight in non-carbonate volatiles, mainly residual organic matter from beet juice purification and bound water. Calcination CO₂ from the carbonate itself accounts for about 31–38%, based on the measured CaCO₃ range. In a kiln, the non-carbonate fraction burns off in the preheater rather than contributing CaO, so it should be included in raw-mix design and in total hydrocarbon and CO monitoring during trials. The organic fraction is beet-derived (biogenic), and its fuel value is negligible (170 BTU/lb, dry basis). The as-shipped figure assumes 10% moisture, the level of the air-dried lab sample. In the finish mill or in concrete, PCC is not heated and these volatiles do not apply.
What PCC fineness is worth at each point of use
| Where PCC goes | What the plant needs today | What PCC brings |
|---|---|---|
| Raw mill (kiln feed) Cement | Quarried limestone blasted, crushed, and ground to raw meal, typically about 85% passing 90 µm, with coarse calcite kept low for burnability. | About 90–94% passing 75 µm on arrival and no coarse calcite, so it can skip crushing and raw grinding. |
| Finish mill (Type IL) Cement | Limestone ground finer than clinker to deliver filler and packing benefits. Type IL is typically ground about 100 m²/kg Blaine finer than the companion Type I/II. | Dispersed median about 12–15 µm, in the same range as portland cement (about 12–16 µm), with roughly twice cement’s share of particles finer than 2 µm, already made, at no kWh per ton cost. |
| Mix design Ready-mix concrete | Fine carbonate filler that improves particle packing and early-age hydration without hurting strength. | At 5% replacement of Type IL cement in mortar, 28-day strength rose 8.1% and drying shrinkage fell 8.9%. |
What one ton of PCC replaces
PCC is a supplemental calcium source, not a pound-for-pound swap. About 1.39 tons of PCC as shipped deliver the calcium carbonate in one ton of 96% limestone. The minor constituents PCC carries, including residual organic matter from beet juice purification, should be included in your mix design and, for kiln feed, in trial emissions monitoring.
As-shipped values assume 10% moisture and 77% CaCO₃ (dry basis), the average of eight lab samples.
PCC sources: Energy Laboratories analyses of Western Sugar Fort Morgan PCC (October 2017 and January 2018, eight samples; CaCO₃ 70.3–85.6% dry basis, average 77%). SK Geotechnical sieve and hydrometer analyses of dispersed material (2018, three samples; 89.5–93.9% passing No. 200; median about 12–15 µm; about 20–25% finer than 2 µm in two of three samples). Standard Laboratories analysis of Western Sugar Billings stockpile PCC (2025; LOI by ASTM D7348 on a sample air-dried to about 10% moisture, reported on a dried basis). South Dakota State University SEM image analysis (2026; median of agglomerated clusters about 22 µm) and mortar testing (2026). CaO is calculated from CaCO₃. Comparison values for portland cement, Type IL, and raw meal are typical published values from ASTM C150 and C595, Ferraris, Hackley, and Aviles (2004), and the Portland Cement Association (Tennis et al., 2024). PCC from the Lovell and Scottsbluff factories comes from the same process but has not been separately characterized here. All values are typical, not guaranteed.
Estimating savings at your plant
PCC saves money when its delivered cost per ton is below 72% of what your limestone costs you.
Delivered cost is the PCC price at our factory plus your freight, plus any drying cost. The 72% reflects the 0.72 tons of 96% limestone that each ton of PCC replaces.
Break-even delivered cost of PCC
| Your limestone cost, delivered to the process | $15/ton | $20/ton | $25/ton | $30/ton |
|---|---|---|---|---|
| PCC breaks even at a delivered cost of | $10.83 | $14.44 | $18.05 | $21.66 |
Worked example: replacing 10,000 tons of limestone a year
Limestone at $20 per ton delivered to the process, PCC at no charge at the factory, no added drying cost, and $50,000 in one-time integration capital. This takes about 13,850 tons of PCC as shipped (12,470 dry tons), or roughly 462 truckloads.
| Your freight rate per ton of PCC | Limestone avoided | Freight | Yearly benefit | Payback | 5-year net |
|---|---|---|---|---|---|
| $5 | $200,000 | −$69,264 | $130,736 | 4.6 months | $603,680 |
| $10 | $200,000 | −$138,528 | $61,472 | 9.8 months | $257,360 |
| $12 | $200,000 | −$166,234 | $33,766 | 17.8 months | $118,832 |
| $14.44 (break-even) | $200,000 | −$200,000 | $0 | Not reached | −$50,000 |
Run the numbers for your own plant
- PCC needed (as shipped) = limestone to replace × your limestone CaCO₃ ÷ (PCC CaCO₃ × (1 − PCC moisture)). At 96%, 77%, and 10%, that is limestone tons × 1.385.
- Yearly benefit = limestone tons × limestone cost − PCC tons × (PCC price + freight) − water tons × drying cost − added handling.
- Crushing emissions avoided = limestone tons × crusher kWh per ton × grid rate. At 1.6 kWh per ton, 10,000 tons avoids 16,000 kWh: about 5.9 t CO₂e at the U.S. average (0.37 kg/kWh) or 7.5 t CO₂e on the Rockies grid (eGRID RMPA, 0.47 kg/kWh).
- Quarry fuel avoided = limestone tons × diesel gallons per ton × 10.21 kg CO₂ per gallon (EPA GHG Emission Factors Hub, 2024).
- Added PCC freight emissions = truckloads × added miles per load ÷ 6 mpg × 10.21 kg CO₂ per gallon. Subtract this from the two lines above for a net figure.
- Scopes: if you run your own quarry, quarry fuel is Scope 1 and crusher electricity is Scope 2. If you buy limestone, both are your supplier’s emissions and count as your Scope 3.
Want an estimate built on your plant’s figures? Request more info and we will run it with you.
Transportation
Backhaul potential
Limestone is a raw input for our factories and for your plant. Where we share a quarry, or our quarries sit close together, PCC can ride on limestone trucks already returning from our factory, and backhaul economics become an advantage.
Dedicated trucks
Trucks run out and back just for PCC. When backhaul synergies don’t apply, freight is the end user’s responsibility.
What PCC changes in your carbon footprint
Goes down
- Drilling, blasting, and hauling at the quarry, reducing Scope 3 upstream emissions from purchased limestone (or Scope 1, where you operate the quarry yourself)
- Primary crushing energy, since PCC arrives pre-processed, reducing Scope 2 emissions from purchased electricity (or Scope 3, where you buy crushed limestone)
- Draw on your limestone reserves, extending quarry life
- Used in the finish mill, PCC as a replacement for clinker has the potential to offset Scope 1 kiln emissions
- Potential clinker reduction in Type IL cement (theoretical)If PCC were interground at the finish mill to displace an additional 5% of clinker, clinker-related emissions would fall by roughly 0.04 t CO₂e per ton of cement (0.05 × about 0.85 t CO₂e per ton of clinker). This extrapolates from mortar testing in which PCC replaced 5% of Type IL cement and 28-day compressive strength rose 8.1% (Teymouri & Acharya, 2026). PCC concrete is now being demonstrated in the field (Idaho State University, 2026). Total limestone content above 15% falls outside ASTM C595 limits for Type IL.
Used as kiln feed, PCC releases the same calcination CO₂ as quarried limestone, so its carbon case there rests on avoided quarrying, crushing, and hauling, net of PCC freight. Used in the finish mill in place of clinker, PCC has the potential to offset Scope 1 kiln emissions.
Approved uses
Each state’s authorization carries its own conditions and periodic testing. Review the current authorization for your state before use.
Research on PCC as a filler in concrete
PCC in finished cement and concrete has moved from the lab to its first field pour. Across studies, about 5% replacement gives the best strength; higher replacement levels trade strength for lower cement content.
South Dakota State University, 2026
Western Sugar PCC replaced part of the Type IL cement in mortar. 28-day compressive strength:
At 5%, PCC also gave the lowest drying shrinkage (8.9% below the reference) with a small reduction in flow. SDSU describes this as a preliminary feasibility check in mortar; testing in concrete is planned.
Strength with PCC compared with conventional cement
| Study | Material tested | Cement replaced | Control | With PCC | Change |
|---|---|---|---|---|---|
| SDSU, 2026 Western Sugar PCC | Mortar, 28 days, ASTM C109, Type IL cement | 5% | 5,229 psi | 5,654 psi | +8.1% |
| Gharieb & Rashad, 2020 Beet carbonation lime | Cement paste, 28 days | 5% | Reference | Higher | +4.8% |
| Idaho State, 2023 Sweetcrete | Concrete, 28 days, w/c 0.44 | 25–30% | Conventional | ≥4,000 psi | Meets target |
No concrete-scale result at 5% replacement has been published yet. The Idaho State concrete work tested higher replacement levels and found up to 30% of the cement could be replaced while still meeting a 4,000 psi (28 MPa) target.
Idaho State University, 2023–2026
Sweetcrete, a concrete made with PCC from Amalgamated Sugar’s Paul, Idaho factory, moved from the lab to its first field pour in spring 2026: a 9-foot by 71-foot pad, 21.5 cubic yards, placed by Kloepfer Inc. in Burley, Idaho. Read the ISU announcement.
References: Teymouri, M., & Acharya, P. (2026). Preliminary assessment of precipitated calcium carbonate as a partial cement replacement [Report for Western Sugar Cooperative]. South Dakota State University. Gharieb, M., & Rashad, A. M. (2020). An initial study of using sugar-beet waste as a cementitious material. Construction and Building Materials, 250, 118843. https://doi.org/10.1016/j.conbuildmat.2020.118843. Phuyal, K., Mashal, M., et al. (2023). A sustainable and environmentally friendly concrete for structural applications. Sustainability. Idaho State University. (2026, April 27). From byproduct to breakthrough: ISU’s Sweetcrete hits the field. isu.edu.
Estimates for planning purposes only, based on typical material test results. Actual results depend on your mix design, plant trials, PCC moisture at loading, actual road routes, and freight arrangements. Use of PCC requires the current beneficial use authorization for the state where it will be used. Request More Info